Review test results for submitted samples of decorative elements, surface coating, Kley installation adhesive and foam, examined by independent Thai institutions in 2015–2016. The original laboratory reports are provided for reference.
Mechanical Strength of Decorative Cornices
Tests measured compressive strength, flexural strength and initial surface absorption of lightweight cornice samples.
Compression: 0.26 MPa · Flexure: 0.43 MPa
TIS 1505-2541 · ASTM C1185-03 · BS 1881-208:1996
Department of Science Service · Report L58/05622.1
View report (PDF) ↗
Accelerated Weathering
After one week of cyclic UVA-340 exposure and condensation, no cracking, blistering or chalking was observed on the submitted specimen.
8 h UVA-340 (60 °C) / 4 h condensation (50 °C)
ASTM D4329, Cycle A
Department of Science Service · Report L58/05642.1
View report (PDF) ↗
Kley Adhesive Bond Strength
Adhesive bonding between concrete and a lightweight cornice specimen was measured two days after application.
Bond strength: 0.10 MPa at 2 days
ASTM C952-02
Department of Science Service · Report L58/03246.1
View report (PDF) ↗
Foam Sample Exposed to Flame
The report recorded ignition during direct flame exposure followed by flame extinction under the conditions described.
Vertical and horizontal test orientations
ASTM D568 · ASTM D635
KMUTT · Report dated 27 April 2016
View report (PDF) ↗